Komposisyon ng Kemikal sa %, Invar
tatak | Komposisyon ng kemikal | ||||||||
Ni | Fe | C | P | Si | Co | Mn | Al | S | |
≤ | |||||||||
4j42 | 41.5~42.5 | Bal | 0.05 | 0.02 | 0.3 | - | 0.80 | 0.10 | 0.02 |
4j45 | 44.5~45.5 | Bal | 0.05 | 0.02 | 0.3 | - | 0.80 | 0.10 | 0.02 |
4j50 | 49.5~50.5 | Bal | 0.05 | 0.02 | 0.3 | 1.0 | 0.80 | 0.10 | 0.02 |
4j52 | 51.5~52.5 | Bal | 0.05 | 0.02 | 0.3 | - | 0.60 | - | 0.02 |
4j54 | 53.5~54.5 | Bal | 0.05 | 0.02 | 0.3 | - | 0.60 | - | 0.02 |
Mga pangunahing pisikal na pare-pareho at mekanikal na katangian ng haluang metal:
tatak | Thermal conductivity | Tiyak na kapasidad ng init | Densidad | Electric resistivity | Curie point |
4j54 | 18.8 | 502J | 8.28 | 0.42 | 530 |
Karaniwang pagpapalawak ng character(10 -6 / ºC ) | ||||||||
Saklaw ng temperatura | 20~100 | 20~200 | 20~300 | 20~350 | 20~400 | 20~450 | 20~500 | 20~600 |
Koepisyent ng pagpapalawak | 10.7 | 12.7 | 10.7 | 10.7 | 10.8 | 10.3 | 10.8 | 11.2 |
4 j54 haluang metal ay pangunahing ginagamit para sa at mika, malambot na sealing glass